In an electroplating shop, a standard chiller can fail within months. The compressor is usually fine; the condenser tubes pit through, the evaporator leaks, or the control cabinet terminals turn black. The cause is the environment: hydrochloric, sulfuric and chromic acid mists, plus cooling water at pH 2–3.
The specification therefore starts with the material and the layout, not with the cooling capacity. This article maps the corrosion sources, compares wetted materials, explains why a closed cooling loop is preferred, and gives a load calculation for a plating shop.
The examples are illustrative. Final selection must use the bath chemistry, ventilation data and the manufacturer’s corrosion guide.
1. Where the corrosion comes from
| Source | Corrosive medium | Affected parts |
|---|---|---|
| Shop air | HCl, H2SO4, chromic acid mist | Control cabinet, fins, casing |
| Cooling water | Low pH, chloride | Condenser tubes |
| Chilled water | Acid or alkali ingress from bath | Evaporator, pump, piping |
| Floor | Acid spill, wet atmosphere | Base, cable tray |
The plating type changes the severity. Chromium and nickel plating use strong acids and produce heavy mist; zinc and copper are milder; cyanide plating adds a separate safety requirement. Get the bath composition and ventilation data before choosing materials. “Electroplating shop” alone is not a specification.
2. Wetted materials: titanium is the default, not universal
| Material | Acid / chloride resistance | Typical use | Relative cost | Limit |
|---|---|---|---|---|
| Copper | Poor | Clean water only | 1.0 | Not suitable for plating |
| 316L stainless | Moderate | Piping, frame, low-chloride water | 1.6 | Pits in high chloride |
| Titanium | Excellent | Condenser and evaporator tubes, plates | 3.5 | Not resistant to HF |
| Hastelloy | Excellent | Sulfuric / mixed acid, HF | 6.0 | High cost |
| PTFE-lined / graphite | Excellent | Strong acid, special heat exchangers | 2.5 | Lower heat transfer |
Titanium is the mainstream choice. Its oxide film resists chlorides and most inorganic acids, and a titanium tube condenser can last ten years in a plating shop where copper fails in months. Titanium is not resistant to hydrofluoric acid; if the bath contains HF, use Hastelloy or PTFE-lined equipment.
Plate or shell-and-tube? A plate heat exchanger is compact and efficient, but the gaps are narrow and the gaskets are attacked by acid. A shell-and-tube titanium exchanger is easier to clean mechanically and tolerates particles. For plating baths with sludge or scale, choose shell-and-tube.
3. Air-cooled or water-cooled
Air-cooled in the shop. The fins are exposed to acid mist and corrode. A coating slows it but does not stop it. If the unit must be in the shop, use coated fins, a corrosion-resistant casing and a positive-pressure cabinet, and accept a shorter life.
Water-cooled with an open tower. The tower water is exposed to acid mist, and the pH falls. Even a titanium condenser is protected, but the tower, fill and basin corrode. Water treatment is difficult because the contamination is continuous.
Water-cooled with a closed tower. The process water stays inside a closed circuit; only the spray water evaporates. The process water is not exposed to acid mist, so its pH and chloride remain stable. This is the recommended configuration for a plating shop.
Chiller in a separate room. Locate the chiller outside the plating hall, with the intake on the clean side and away from the exhaust path. This single measure is more effective than any coating. If the chiller must be inside, isolate it with a partition and pressurize the room.
4. Load calculation
The cooling load comes from three sources: current heat, reaction heat and ambient heat. Current heat dominates.
Current heat. For a bath at voltage V and current I, the electrical heat is approximately V × I. A 12 V, 5,000 A bath releases 60 kW. Add reaction and ambient heat, and the cooling load is 70–80 kW.
Margin. Add 20% for summer conditions and the lower efficiency of titanium compared with copper. Select at 1.2 × the calculated load.
Simultaneity. Multiple baths do not all run at full load. Use a 0.7–0.8 factor for the total, and install multiple units for staging and standby.
Standby materials. Do not downgrade the standby unit to copper because “it rarely runs”. When it starts, the acid mist and low-pH water are still there, and it will fail just as quickly. Specify the same materials for duty and standby.
| Bath | Voltage / current | Current heat | With margin |
|---|---|---|---|
| 12 V, 5,000 A | 12 V / 5,000 A | 60 kW | 72–80 kW |
| 8 V, 4,000 A | 8 V / 4,000 A | 32 kW | 38–43 kW |
| 6 V, 3,000 A | 6 V / 3,000 A | 18 kW | 22–25 kW |
5. Materials configuration
| Part | Standard | Plating-shop specification |
|---|---|---|
| Condenser tubes | Copper | Titanium |
| Evaporator | Stainless plate | Titanium plate or shell-and-tube |
| Chilled-water piping | Galvanized steel | 316L or UPVC |
| Pump | Cast iron | 316L or PTFE-lined |
| Casing | Painted steel | 316L or heavy-duty coating |
| Fins (air-cooled) | Aluminum | Coated aluminum or copper fins |
| Control cabinet | Standard | Positive-pressure ventilation + coating |
| Terminals | Copper | Tinned |
Positive-pressure ventilation is worth specifying separately. A small filtered air supply keeps the cabinet at a slight positive pressure, so acid mist cannot enter. It costs far less than a fully sealed corrosion-proof cabinet and is easier to maintain.
6. Operation and maintenance
Check chilled-water pH weekly. A falling pH means bath liquid has entered the chilled-water circuit. Titanium may survive, but the pump, piping and seals may not. Investigate the leak immediately.
Clean the exchanger. Plating water deposits metal salts and scale. Shell-and-tube units can be brushed mechanically every six months; plate units need cleaning when the pressure drop rises. Do not use hydrochloric acid for cleaning without checking all wetted materials; titanium resists chloride, but 316L and other components may not.
Inspect coatings and terminals. Bubbles in the casing coating should be repaired. Black terminals indicate acid mist ingress; check the positive-pressure fan and filter.
Protect the base. Acid spills travel along the floor and attack the concrete base. Apply an epoxy coating, provide a containment curb, and keep the cable tray off the floor.
7. Boundaries and safety
Hydrofluoric acid requires Hastelloy or PTFE; titanium will fail. Cyanide plating requires separate ventilation and leak detection because acid contact can release toxic gas. Baths above 60 °C need a high-temperature chiller; a standard comfort chiller may not handle the evaporating temperature. If the shop cannot provide a separate room or clean air intake, the equipment life will be shorter regardless of material; include that in the lifecycle cost.
Frequently asked questions
Why do electroplating chillers corrode?
Acid mist from plating baths, chloride rinse water and aggressive cleaning agents attack coils, headers and frames. Condensation on a cold coil concentrates acid, so corrosion is often worst at the evaporator and drain pan, not in the water circuit.
Which materials should be used?
PP or PVDF wetted parts, PTFE-lined tubes, titanium or 316L where appropriate, and epoxy-coated frames. The choice depends on the bath chemistry: sulfuric acid, hydrochloric acid, chloride and hexavalent chromium need different answers.
How is the cooling load calculated?
Use bath volume, set temperature, heat from rectifiers and pumps, surface losses and the required pull-down time. Add the rinse and ventilation load. Do not size from tank volume alone; rectifier heat often dominates.
Can one chiller serve several baths?
Only with hydraulic separation and independent temperature control. Baths at different temperatures need mixing valves or separate circuits. A single loop can starve the hottest bath and cause quality rejects.
How should acid mist be controlled?
Enclose or hood the baths, exhaust near the surface, and keep the chiller away from the plume. A corrosion-resistant coil coating helps, but source capture is more effective than cleaning later.
What maintenance is needed?
Inspect coils and drains for corrosion, clean according to the bath chemistry, check refrigerant leaks, and replace filters. Keep a corrosion coupon in the worst location and review it quarterly.
Can I use a standard chiller with a coating?
Sometimes, for light duty. For constant acid mist or chloride, a coated standard coil may fail at welds and drains. Use a unit designed for corrosive environments, or isolate the coil with a heat exchanger.
What should be specified?
Bath chemistry and concentration, required temperature and tolerance, heat load, ambient acid mist, materials, access for cleaning and the acceptable downtime. Provide a corrosion coupon test if the chemistry is unusual.
Related reading
Electroplating chiller corrosion · Chiller expansion valves · Cooling tower and chiller selection